POLYASPARTIC TECHNICAL ARTICLES

Polyaspartic Polyurea Technical Articles

How Is Gaodun N600 Outdoor Flake Flooring Installed? Concrete Sealing, Full Flake Broadcasting and Clear Topcoating

Gaodun N600 outdoor decorative flake flooring is used on qualified concrete decorative floors. This guide uses Gaodun’s confirmed construction route: after concrete grinding and crack repair, use N600 substrate sealing, then use N600 for body coat and full broadcasting of decorative flakes on the wet film, after recycling excess flakes, trimming and vacuuming, use N200 clear topcoat. If dampness, substrate surface dusting, active cracks or reverse drainage fall continue to recur, the cause should be identified and dealt with first. This article explains the release conditions, on-site inspection and work suspension points of each process, and attaches a start-up and acceptance inspection form to help owners and construction leaders check site trial, partition succession, topcoat and opening conditions. If the terrace assumes the waterproof function of the building, the project's waterproof structure and acceptance criteria must be separately checked. Readers can also use this to determine which process should be used to check for chipping, pinholes and color differences.

Article contents (10 sections)

Installing Gaodun N600 outdoor decorative flake flooring

Gaodun’s N600 decorative flake flooring uses N600 for both the sealer and the flake-bearing midcoat, and N200 for the clear wear-resistant topcoat. On sound, clean, dry outdoor concrete with adequate drainage, seal the prepared surface with N600. Once the sealer meets the recoating requirements, apply the N600 midcoat and broadcast decorative flakes into the wet film. When the midcoat is ready, remove loose flakes, trim raised edges and vacuum before applying the N200 topcoat. Allow the floor to cure before acceptance. Resolve persistent dampness, surface dusting, moving cracks or drainage that slopes the wrong way before coating. Record batches, mix quantities and application details separately for the two N600 coats. For a terrace over occupied space, verify the primary waterproofing and its details separately. Check each grade’s intended use on its product page and follow the project’s approved system documents. [1][2]

Applicable conditions | Which concrete floors can enter the site trial stage?

This guideline applies to patios, outdoor walking areas and patio concrete decking surfaces where conditions have been confirmed. Before starting work, confirm the planned use and record whether there will be frequent wet cleaning, moving furniture, vehicle traffic, or frequent water accumulation. The method of use determines the anti-skid, wear-resistant and maintenance requirements of the finished surface. The general procedures in this guide are geared towards decorating a pedestrian scene. For vehicle operation, long-term water immersion or special medium working conditions, the compatible system and engineering verification should be checked separately.

The substrate should be overall stable, and the old leveling layer and local repairs should be checked for hollow-sounding areas, surface dusting, powdering and obvious height differences. For cracks, structural joints and expansion joints that continue to open and close, the displacement and details should be confirmed first. If drainage is poor, reverse drainage falls at the door, or water accumulates in low places, the drainage structure needs to be adjusted first. If there is a use space under the terrace, the existing waterproofing and details design should be checked first, and then the responsibilities of the decorative flake floor in the overall structure should be determined.

Start-up inspection | First check where the water comes from, and then check whether the concrete surface can be painted

Before starting work, mark out the low points of water accumulation, drain openings, cracks, old repair areas and shaded areas on the plan map. Check recent rainfall, cleaning or long-term recurring dampness, focusing on seams, doorways and wall bases. When screening concrete for signs of capillary water is required, the plastic film method of ASTM D4263 may be considered per project plan. This method is used to indicate the presence of capillary water. The inspection method corresponding to the selected system requirements must still be used for project release, and the measurement points and results must be recorded. Substrate sealing should be suspended when encountering continued humidification or water accumulation of unknown origin. [3]

The person in charge of construction should also check the technical data sheet (TDS) and safety data sheet (SDS) of the selected model to confirm the identification of the two components, construction environment, operable time and protection requirements. Divide the construction area according to the actual operating time, and arrange the connection of mixing, coating and spreading personnel. Allow time for recoating, curing and rainproofing. If condensation, rainfall or significant dust occurs during the planned construction period, the relevant processes should be stopped and the completed areas should be reviewed.

Compatible system and materials | The roles of the sealing coat, body coat and topcoat

Table 1
process or material Responsibilities in this N600 compatible system Confirm before starting work
N600 sealer Wets and seals the prepared concrete Check substrate absorption, product identity, the compatible thinner and the approved sealing procedure
N600 flake-bearing midcoat Holds decorative flakes broadcast into the wet N600 coat Verify the matched A and B components, application rate and time available to broadcast the flakes
decorative flakes Create color, pattern and surface texture Color number, batch matching, site trial appearance and full broadcasting method
N200 clear topcoat Protects the trimmed and cleaned flake layer Confirm compatibility, finished texture and intended traffic

The site trial should include the main surface, wall or door edges, and representative repair areas. The owner and construction leader will work together to review color, texture, joints between application areas and wet-traffic requirements. If granular materials such as white fused alumina are selected for the project, first conduct a site trial with complete topcoat to confirm the granular specifications, adding method and usage effect. The granules will change the surface texture and cleaning difficulty. Procurement and acceptance inspection should be based on the actual compatible system site trial.

Construction steps | How to check after each step

Grind and clean the concrete and repair stable cracks. Remove laitance, loose material, old coating residues and contaminants that impair adhesion as specified in the work plan, then vacuum up the dust. Use compatible repair materials for stable cracks and gaps, and allow them to cure as specified before coating. Check the edges of the repairs for soundness and look for surface dusting or uneven absorption. If the concrete still powders after grinding, oil continues to seep out, or cracks continue to open and close, stop work and reassess the substrate. Follow the project joint detail wherever a joint must accommodate movement.

The second step is to use N600 for substrate sealing. Mix the materials with the substrate sealing process according to the component ratio confirmed in this project. Fill in the actual weight of component A, component B and compatible thinner respectively in the record sheet, and indicate the calculation basis for the addition ratio. Apply evenly and observe the absorption status of the substrate, and check for coating leakage, pile-up, continued foaming and uneven drying and wetness. Construction records separately list the amount of mix, thinner used and area in the area. After the technical documents and on-site conditions confirm that recoating is possible, do the body coat. When local bubbling occurs repeatedly, the surface is still sticky or contaminated by rainwater, the cause should be identified and the recoating conditions should be confirmed.

The third step is to apply N600 to the body coat and full broadcasting of decorative flakes. Ingredients are batched according to the area that can be completed, and mixing, rolling and spreading are arranged within the approved construction window. When the supporting layer is still in a spreadable state, broadcast evenly and fully, paying attention to corners and joints. Check for exposed midcoat, streaks or local piles of flakes. If the supporting layer has lost its effective adhesion ability, suspend the spreading of chips in this area and handle it according to the compatible system plan. Zoning boundaries should incorporate natural boundaries or predetermined construction lines.

The fourth step is to recycle excess flakes, trim them and vacuum them. After the supporting layer reaches the workable state, remove excess flakes that are not firmly adhered, trim the warped and protruding edges, and vacuum up surface and corner debris. Check whether bonded flakes detach in patches, whether the joint edge is raised and whether areas along walls or at doorways were missed during flake broadcasting. When it is found that the supporting layer is soft or sticky or the decorative flakes main surface area has fallen off, stop the topcoat and first check the curing, spreading time and substrate status.

The fifth step is to use N200 to make clear topcoat. Check the A and B identification, proportion and measurement method of the corresponding batch of N200, batch ingredients according to topcoat technical documents, and record the mixing start time, dosage and construction area. If anti-skid particles are added according to project requirements, the particle model, particle size, addition standard and actual dosage should be indicated. The texture should be checked with the approved site trial before expanding the construction. When topcoating, carefully check the edges, wall bases and joints between application areas, and observe for whitening, pinholes, sags, exposed tips or piles of materials. When condensation, rain contamination, or the anti-skid texture is significantly filled in, pause the affected area and re-inspect it. Opening will confirm the conditions for walking, placing furniture and cleaning and receiving water according to the actual curing situation and project acceptance inspection.

Zone handover | How to reduce obvious transitions at doorways and long passages

Take a patio walk with corners and thresholds as an example. You can first mark the starting and ending locations of each construction area and the exit routes for personnel, and try to arrange long passages that are prone to color bands in the same continuous operation area. When handing over each area, record the starting coating, spreading and final completion positions of the supporting layer. If the personnel or materials cannot keep up, stop at the scheduled construction line, retain the processing conditions, and record the reason for the interruption. Before the next construction, check the curing status, edge treatment and overcoating conditions allowed by the corresponding product in the previous area, and first confirm in a small area whether the joint can meet the site trial requirements.

Acceptance inspection | Appearance, anti-skid, drainage and opening are inspected separately

The acceptance inspection first checks the partition, batch, material and construction records, and then checks the color, splice and topcoat integrity. ISO 2808:2019 lists wet film and dry film thickness measurement methods respectively, and Appendix B involves rough surfaces. You should first agree on whether to measure the single layer or the total thickness, as well as the method suitable for the actual substrate and decorative flakes texture. If it is agreed to use ASTM D7234-22 to test the coating adhesion on concrete, the measured values ​​and damage locations should be recorded at the same time, and the test points should be repaired. [4][5]

In daily walking areas, focus on checking doorways, slopes, and locations prone to water accumulation. After the appearance meets the site trial requirements, wet slip resistance and drainage should still be checked as agreed. Before opening, the construction manager will record the curing and completion status of the site, and confirm the conditions for walking, placing furniture, cleaning or receiving water. Cleaning and access arrangements are carried out in accordance with applicable information and project acceptance inspection.

Common Defects | What to check first when there are peeling pieces, pinholes or continuous color difference

For flake loss, first establish whether it occurred before the clear topcoat was applied or after the floor entered service. If flakes detached in patches before topcoating, check whether the supporting midcoat cured, whether it was still tacky enough when the flakes were broadcast and whether only loose surface flakes were removed. After the topcoat is partially cracked or peeled, you should identify whether the damage is located in the topcoat, decorative flakes layer or the concrete interface, and then confirm the scope of repair. Before repair, you can try it out in a representative position to check the overlap, appearance and texture.

When pinholes are concentrated in the repair area, first compare the substrate absorption, substrate sealing continuity and construction environment of the area. If the color difference is distributed along the construction zone, check the batch mixing and spreading time of decorative flakes and the amount of topcoat. If there is a difference in reflection between the shadowed area and the sunny area, it should be compared with the site trial under the agreed observation conditions. After the repair is completed, re-check the inter-layer connection, traffic and drainage of the corresponding area.

Start of construction and acceptance inspection checklist

Table 2
Check time point Release requirements field notes
Before grinding the concrete Drainage, crack properties and recurring dampness have been checked, and there are treatment plans for doubtful points. Floor plan, details photos, start-up inspection
before substrate sealing The concrete and repair layer are firm, clean and meet the construction conditions. Substrate check, environment record, TDS version
Before broadcasting decorative flakes Check that the N600 sealer is ready for recoating. Coordinate application of the N600 midcoat with broadcasting the flakes while the film is wet. Batch, area, application rate and recoating record
before topcoat The decorative flakes are fixed, excess flakes and dust have been removed, and the edges can be inspected. site trial, succession and edge photos
Before delivery Appearance, membrane layer, drainage and traffic meet the project agreement Acceptance inspection point, re-inspection and opening confirmation

References

[1] Shenzhen Gaodun New Materials Co., Ltd.: "Gaodun polyaspartic polyurea floor N-600", official product page, no version date marked. Used to check floor usage. Access date: 2026-11-06. Source (gao-dun.com)

[2] Shenzhen Gaodun New Materials Co., Ltd.: "Gaodun polyaspartic polyurea waterproof coating N-200", official product page, no version date marked. Used to check the positioning of transparent protective topcoat. Access date: 2026-11-06. Source (gao-dun.com)

[3] ASTM International: "ASTM D4263-24 — Standard Practice for Indicating Moisture in Concrete by the Plastic Sheet Method", 2024 edition. Only the disclosure scope and purpose were checked, and the full text of the standard was not read. Access date: 2026-11-06. Source (store.astm.org)

[4] International Organization for Standardization (ISO): "ISO 2808:2019 — Paints and varnishes — Determination of film thickness", 2019 5th Edition. Only the official introduction was checked and the full text of the standard was not read. Access date: 2026-11-06. Source (iso.org)

[5] ASTM International: "ASTM D7234-22 — Standard Test Method for Pull-Off Strength of Coatings on Concrete Using Portable Pull-Off Adhesion Testers", 2022 edition. Only the disclosure scope and purpose were checked, and the full text of the standard was not read. Access date: 2026-11-06. Source (store.astm.org)