POLYASPARTIC TECHNICAL ARTICLES

Polyaspartic Polyurea Technical Articles

Why Does Polyaspartic Polyurea Blister, Peel or Crack? Reducing Failure Risks Before Buying

Blistering, peeling or cracking in polyaspartic polyurea coating may involve material formula, batch status, substrate conditions, compatible system compatibility and construction curing. A photo alone is often not enough to determine cause and liability. From the perspective of an R&D and manufacturing enterprise, Gaodun explains the differences between several types of defects, the inspection information that needs to be retained, and the preventive conditions that can be verified before purchasing, helping consumers make informed purchase and repair judgments. After an abnormality occurs, it is not advisable to add additional curing agents, catalysts or solvents by yourself, nor is it advisable to cover the new coating directly to seal unconfirmed problems in the lower layer. The instructions, environment and construction records should be checked first before determining whether to continue curing, testing or clearing and redoing.

Article contents (11 sections)

1. If a defect occurs, first confirm where and when it occurred.

Consumers often worry about: After spending money to make waterproofing, bubbles, peeling or cracks appear later. Is the material useless?

These phenomena require attention, but they belong to different failure manifestations. There may be multiple causes involved in the same look, and there may be both material and site issues on the same project.

Gaodun recommends recording three pieces of information first: whether the defect occurs during construction or after use, where it is concentrated, and whether it occurs inside the coating film, between two coatings, or between coating and substrate.

Table 1
performance main viewing direction What needs further verification?
Surface vesicles, pinholes or crater-like defects Gas escape and leveling state during film formation Venting, Mixing, Viscosity and Application Windows
Blistering of the coating in service Partial bulge or interface separation of coating Moisture source, adhesion, medium and material status
Coating peeling or separation between coats Location of separation to identify Locate the failure plane in the substrate, within a coat or at an interface. Compare it with surface preparation and recoating records.
crack or tear Location and depth of cracking to inspect Identify the affected layer and review local movement, film thickness and curing records. A photo alone cannot establish the cause.
The coating remains tacky or has patches that have not dried Local state of cure to investigate Record the model, batch number and affected area. Check actual weights, mixing, temperature and cure time against the current TDS.

This table is used to determine the direction of investigation, not to make a diagnosis directly based on appearance.

2. Blistering is not necessarily caused by moisture, it may also come from substrate exhaust.

Concrete has pores. When the coating is initially cured, if the substrate heats up, the gas in the pores may escape and pass through the unstable coating film, forming small bubbles or pinholes.

Sherwin-Williams' public technical information specifically discusses the relationship between concrete pores, substrate heating and exhaust defects, and points out that the shape of defects is affected by the composition, thickness and curing stage of the coating. Sherwin-Williams

In addition, air is involved in stirring, mismatch between material defoaming and leveling, and improper single-pass coating may also affect film formation. If moisture exists, it is also necessary to consider the impact of the interface and the possibility of side reactions between isocyanate-containing components and water to produce gas.

Therefore, "seeing bubbles means there is water on the substrate surface" is not sufficient. "Reactive materials are not afraid of moisture" cannot be used as a basis for construction.

Before purchasing, you should ask whether the concrete needs to be sealed, how the substrate and environment are inspected, and the allowable dosage for a single pass. The construction time needs to be arranged based on the substrate temperature change, dew point and product window. You cannot mechanically think that it can be solved by just changing it to the evening.

3. If the bulge appears after use, check where the water comes from and why the interface is separated.

Small bubbles during construction should not be confused with bulges that gradually grow after use.

Later bulges may be related to moisture in the substrate, external water intrusion, insufficient local adhesion, or other interface problems. Appearance after exposure to rain, high temperatures, or standing water does not alone prove one cause.

You should check whether the bulges are concentrated in brick joints, cracks, depressions or close edges, and whether there is recurring dampness, salt precipitation, leakage paths and old layer detachment around them.

Gaodun suggested that the overall distribution and local photos be retained first, and then relevant technical personnel determine whether local sampling inspection is needed. Blindly puncturing all bulges may destroy the inspection information and may also increase water inlet channels.

Continuously recurring dampness or water entering the structural layer, if not treated, may make it difficult to obtain stable results by simply covering the bulge with another layer of material. Restoration requires consideration of both the water source and the interface.

4. Peeling first looks for the failure surface: does the coating fall off, or does the substrate fall off together?

Peeling is often simply called "not sticking", but it actually requires distinguishing the location of failure.

When the coating separates from a clean brick or concrete surface, the wetting, contamination, surface treatment, water content and compatible system should be checked; when two coatings separate, the recoating window, inter-layer contamination and compatibility should be checked; if there is loose mortar or old paint on the back, the strength of the substrate or old layer itself should also be checked.

Before painting, check that the substrate surface is clean, dry and firm. When it comes to retaining the old layer, determine the mechanical treatment, cleaning and small area adhesion verification methods according to the requirements of the selected system.

For tiled terraces, "the coating is well combined with the brick surface" and "the tile itself is firm" need to be confirmed separately. The material does not replace the treatment of loose old bricks or powdered substrate on the main surface area.

Adhesion testing should also record the location of damage. Analyzing a value together with the corresponding damage pattern is often more meaningful than displaying the value alone.

5. Cracking should not only look at elongation, but also how the substrate moves.

Just because a coating film can stretch does not mean that it can span cracks of any width and speed.

When reading a tensile report, first identify whether the specimen was a free film. For roof cracks, corners and joints, consult the product instructions and the proposed joint detail. For example, page 4 of Gaodun’s Simplified Chinese N700 TDS V2.6 identifies details requiring repair or reinforcement. That page gives no allowable joint movement.

Map the coating cracks against existing substrate cracks, roof details and the open roof area. Compare film thickness and application and curing records for cracked and intact areas. A photograph alone does not establish the cause.

For cracks that continue to develop, the cause should be identified first; for expansion joints, details should be designed to allow displacement. We cannot rigidly fill all the gaps and then require the main coating to bear all the deformation.

From the perspective of material research and development, Gaodun focuses on the balance of strength, flexibility, low temperature adaptability and long-term stability. Consumers should further verify the model usage and corresponding verification, rather than just comparing the maximum elongation advertised.

6. Problems with the materials themselves must also be included in the scope of investigation

Proper defect analysis should examine both product and site conditions.

For a coating that remains tacky, record the model, A and B components, batch numbers, weights and mixing procedure. Check the application conditions in that model’s TDS. For measured batch properties, match the batch number to its certificate of analysis (COA). Tackiness alone does not establish that the batch failed its specification.

For example, materials suitable for high-hardness topcoat are not necessarily suitable for waterproofing the main body of flexible roofs; products suitable for short-term contact with water cannot automatically be regarded as suitable for long-term immersion.

The same batch of materials has abnormalities in multiple locations with similar conditions, which can be used as clues for further investigation, but it still needs to be verified with retained samples and construction records. Even if local defects occur, material adaptation problems cannot be ruled out based on this.

Gaodun believes that R&D and production companies should participate in inspections and be able to explain component compatible systems, quality records and applicable conditions. The investigation should be based on evidence and should not attribute all problems to construction errors at the outset.

7. If it feels sticky or not dry for a long time, why shouldn’t you apply another layer directly?

Two-component materials need to be thoroughly mixed in specified proportions. Measuring errors, uneven mixing on the walls and bottom of the barrel, moisture or mismatching of components, and unsuitable temperature conditions may all affect curing.

Determine the measurement method, mixing sequence and time according to the model data, and confirm the material mixing and film formation status on the site trial.

But "stickiness" also needs to be distinguished: it is the material that is not fully cured, surface contamination, or a change in surface state after heating. The cause cannot be determined based on feel alone.

After an abnormality occurs, it is not advisable to add additional curing agents, catalysts or solvents by yourself, nor is it advisable to cover the new coating directly to seal unconfirmed problems in the lower layer. The instructions, environment and construction records should be checked first before determining whether to continue curing, testing or clearing and redoing.

Pot life, rain resistance, walkability and adequate cure should be checked separately. The construction arrangement should adopt the corresponding model and the conditions of on-site temperature and humidity.

8. Ask six things clearly before purchasing to reduce the risk of on-site failure.

Consumers can ask suppliers to provide the following information:

Table 2
Things to verify Suggestions
Model adaptation Is this made of waterproof main body, topcoat or corrosion protection material?
substrate surface conditions Old layer, dampness, tiles or surface dusting, what needs to be dealt with first?
metered mixing Is the proportion based on weight or volume? How to control the mixing evenly?
construction window What are the requirements for temperature and humidity, substrate temperature, dew point and pot life?
Separation and curing What are the dosage of each coat, overcoating conditions and rain opening conditions?
Exception handling If there is dryness, bubbles or delamination, how should I keep a sample and contact it for inspection?

After visually observing the surface drying, the substrate temperature, air temperature and humidity should still be measured, and whether construction can be judged according to the dew point temperature difference requirements of the model used.

For important projects, a representative site trial should be conducted first, and records of product batches, proportions, mixing time, weather and dosage should be kept. The site trial should include key details or different substrate surfaces to help confirm whether the specified process can be performed on site.

9. If a problem has occurred, how to organize inspection and repair?

First record the time of occurrence, weather, scope and changes, keep the order, packaging batch, remaining materials and construction records, and then contact the supplier and construction party for joint inspection.

Depending on the problem, select targeted inspections such as moisture content, adhesion, thickness, curing, or material sample retention. When necessary, a third party with appropriate capabilities will be involved to clarify the sampling location and sample source.

Before specifying a local recoat, establish the depth of the defect, whether the substrate is sound, and whether water entry or movement continues. Identify the layers to be treated and confirm preparation and intercoat adhesion for the repair system. Gaodun’s Simplified Chinese N200 TDS V2.6, page 4, states that the topcoat cannot repair structural cracks, hollow areas or water ingress through the substrate.

The repair scope and process should be determined through inspection, and partial verification should be done first. In addition to the appearance after repair, the continuity, adhesion and waterproof functions corresponding to the usage scenario should also be checked.

Shenzhen Gaodun New Materials Co., Ltd. has focused on polyaspartic polyurea systems since 2016. We believe that product reliability needs to be supported by R&D and production control, clear applicable conditions and evidence-based problem handling.

Verify whether the materials match the site before purchasing, keep key records during construction, and identify the location and cause of failure after an abnormality occurs, so that rework can be reduced more effectively and the waterproof corrosion protection function can be restored.

What detection methods can be used for defect inspection?

When inspecting concrete substrate, moisture can be checked according to applicable methods. [1] When conducting pull-off testing on coatings on concrete, the measured values ​​and damage locations should be recorded, and the failure interface should be determined based on the on-site conditions. [2]

References

[1] ASTM International: "ASTM D4263-24 — Standard Practice for Indicating Moisture in Concrete by the Plastic Sheet Method", 2024 edition. See the official public scope of application. Source (store.astm.org)

[2] ASTM International: "ASTM D7234-22 — Standard Test Method for Pull-Off Strength of Coatings on Concrete Using Portable Pull-Off Adhesion Testers", 2022 edition. See the official public scope of application. Source (store.astm.org)