POLYASPARTIC TECHNICAL ARTICLES
Polyaspartic Polyurea Technical ArticlesInterfacial Durability of Polyaspartic Polyurea: Why Is Initial Adhesion Alone Insufficient to Establish Long-Term Bond Stability?
The long-term protection of polyaspartic polyurea relies not only on the coating itself, but also on its stable combination with the substrate and adjacent coatings. The pull-off strength reflects the failure response of the system under specific test conditions and must be explained in combination with the failure location, substrate state and environmental effects. Gaodun combines open standards and research from 2025 to 2026 to discuss evaluation ideas for wet adhesion, temperature difference stress, interface modification and interlayer bonding. Especially confirm that the test actually preserves the wet state. If the immersed sample needs to be dried first, the pull-off dolly is bonded, and the glue is allowed to solidify, the final result may reflect the recovery state after immersion. The report should record the time from sampling to testing, the bonding procedure and the moisture content of the specimen.
Article contents (9 sections)
1. Interpreting pull-off strength and the location of failure
For polyaspartic polyurea coatings on concrete or metal, including multilayer systems, pull-off strength depends on the substrate and test setup. Record where failure occurred to identify which part of the tested assembly limited the result.
ISO 4624:2023 lists three pull-off methods. Method A uses two pull-off dollies and can be used for rigid and deformable substrates. Method B uses a single pull-off dolly and is only suitable for rigid substrates. ASTM D7234-22 is for coating on concrete. The report should describe the method used, the substrate and the location of damage, so that it can be easily determined whether different values can be compared.
The test load passes through the pull-off dolly, adhesive, coating, interlayer interface and substrate, and damage may occur at the weaker locations. Only by identifying the damage surface can we judge which part the numerical value mainly reflects.
| Failure location | What it indicates | Interpretation limits |
|---|---|---|
| between coating and substrate | The interface separated under experimental conditions | Need to combine substrate surface status and sample preparation conditions |
| inside coating | Cohesive failure of coating occurs | The ultimate strength of the interface has not been measured directly. |
| concrete interior | The substrate is destroyed first under test conditions | The numerical value cannot be directly regarded as the ultimate strength of the coating interface. |
| between two coatings | Inter-layer connections become weak points | Overcoating conditions and system compatibility should be checked |
| Within the test adhesive or at its interfaces | Test adhesive layer limits measurement | The validity of the results needs to be judged according to the method used. |
Mixed damage should also record the proportions of different damaged areas.
Gaodun believes that technical reports should also give numerical values, damage locations and test conditions so that the results can be accurately interpreted.
2. Why can’t the results on concrete and metal be ranked directly?
Concrete has pores and surface strength differences, while metals have different oxide layers, surface states, and mechanical responses. Pull-off results for the same coating on different substrates reflect different test conditions.
ASTM D7234-22 clearly points out that different instruments, substrates and loading fixtures may cause variations in strength results.
Therefore, when comparing two formulas, you should try to control:
- substrate batch and surface treatment.
- Actual dry film thickness.
- Curing and conditioning conditions.
- Loading fixture (dolly) size.
- Cutting method and loading conditions.
Even if the results are also expressed in MPa, they are not automatically considered directly comparable.
For Gaodun, adhesion research requires establishing clear correspondence: specific model, specific substrate, specific surface state and specific test method.
3. Why can’t the initial dry state of adhesion replace the wet state and post-aging evaluation?
An initial pull-off adhesion test measures bond strength under the specified dry test conditions after curing. Long-term service also involves moisture ingress, interface swelling, substrate changes and repeated temperature differences.
From the analysis of the interface mechanism, moisture may change the interaction between coating and substrate; for metals, corrosion products may also affect the bonding; for concrete, the water content of the substrate and the surface state need to be considered at the same time. The specific path must be verified by the corresponding system.
Gaodun recommends evaluating them separately:
- Initial dry attachment.
- Wet adhesion after environmental effects.
- Adhesion after drying.
Different explanations are needed between the decline in the wet state and recovery after drying and the still decline after re-drying.
Especially confirm that the test actually retains the wet state. If the immersed specimen needs to be dried first, bonded with the pull-off dolly and waiting for the glue to solidify, the final result may reflect the recovery state after immersion. The report should record the time from sampling to testing, the bonding procedure and the moisture content of the specimen.
The adhesion retention rate also needs to be judged in conjunction with the damage mode. If the front and back are dominated by concrete failure and interlayer separation respectively, a single percentage cannot fully explain the interface changes.
4. How do temperature differences and coating stress affect interface stability?
Thermal expansion, water absorption expansion and deformation capabilities of coating and substrate may be different. When the substrate constrains the coating’s expansion or contraction as temperature or humidity changes, stress may occur near the interface; edges, corners and existing defects require special attention.
From the analysis of interface mechanics, whether local defects expand is related to both the material's ability to withstand interface damage and the stress and load patterns in the actual structure.
Therefore, short vertical pulls alone cannot represent behavior under repeated shear, peeling, or cracking movements. Nor does higher hardness automatically prove better interface durability.
A 2025 "Construction and Building Materials" shear study on the modified polyaspartic polyurea-concrete contact surface found that changes in roughness affected the peak load, energy release and failure mode; within the scope of the study, the damage also gradually involved concrete cracking near the interface.
This result shows that the interface performance needs to be studied in combination with the force mode and substrate response; it does not support the promotion of a certain roughness or treatment method to all substrates.
5. Development direction of interface modification: collaborative design of chemical structure and film formation process
In 2025, "Journal of Elastomers & Plastics" studied silicone-modified polyaspartic polyurea and reported the water resistance and cement mortar adhesion performance of the studied formula.
A study published online on October 27, 2026, used epoxy resin and silane-related components to modify polyaspartic ester resin, and examined changes in reaction, adhesion, mechanics, and thermal stability. Preparation of Epoxy/Silicone-Modified Polyaspartic Resin and Its Effect on Polyurea Properties (2026, publisher's abstract) (journal.hep.com.cn)。
These studies demonstrate that interfacial properties can be tuned through resin and modified structural design. However, just because a silane or epoxy component is added to a formula, it cannot be concluded that an effective chemical bridge has been formed or that it has long-term wet stability.
Gaodun believes that modification studies should also check reaction equivalent, compatibility, curing window, storage state and adhesion after environmental effects.
Whether the improvement can be maintained in the complete formula requires actual measurement; the specific mechanism needs to be supported by structural and interface evidence.
6. Multi-layer system, each interface between layers needs to be verified
After the primer coat, main coat and clear topcoat are combined, the overall protection depends on the coating body and the connections between the layers.
Just because a single product adheres well to metal or concrete does not mean it will perform the same with another coating. Overcoating time, surface contamination, degree of curing and compatible system compatibility may all affect the interlayer connection.
For decorative flakes decorative floors, it is also necessary to pay attention to the wetting and coating of the decorative particles by the resin, as well as the interlayer stability after topcoat.
Therefore, Gaodun advocates verifying the interlayer bonding with a complete system and setting conditions for normal overcoating, close window boundaries, and necessary delayed overcoating.
The specific recoating time and processing method should be verified and determined by the corresponding product and cannot be directly applied across models.
7. How to establish a more interpretable interface durability test?
The following are R&D evaluation suggestions and are not intended to replace specific test standard operating procedures.
| evaluation questions | Recommended to compare | Must be recorded |
|---|---|---|
| Is the initial combination stable? | Multiple samples from the same batch | Numerical distribution, failure surface and abnormal samples |
| Can it remain bonded after the action of water? | Dry, wet and re-drying | Soaking and testing procedures, hydration conditions |
| Does temperature difference affect the interface? | Before and after cycle comparison | Temperature ranges, cycles and checkpoints |
| Is the damage likely to spread? | Choose shear, peel or defect testing by application | Geometry, Loading and Damage Range |
| Is the multi-layer system compatible? | Different overcoating states | Model, thickness and spacing of each layer |
| Whether the experimental results correspond to the application | Engineering substrate surface and standard test board | Substrate surface differences, exposure and maintenance records |
Attention should be paid to the absolute value, degree of dispersion and location of damage at the same time.
If the variation mainly comes from test gel, substrate batch or curing differences, these effects need to be clarified first and then attributed to the formulation. For low modulus or thick film systems, the test applicability and stress conditions should also be checked to avoid directly ranking the results under different test boundaries.
8. Gaodun’s technical stance: Convert adhesion indicators into evidence of interface durability
Shenzhen Gaodun New Materials Co., Ltd. has focused on polyaspartic polyurea systems since 2016, focusing on the research and development, synthesis, formulation and production of Part A and Part B.
Gaodun believes that adhesion research should connect the material structure, substrate state, film formation process and service load. Through testing of corresponding models and complete systems, we will answer step by step:
- Where the bonding occurs.
- How much remains after environmental effects.
- Whether the local damage will continue to expand.
For roofs and terraces, wet adhesion, crack movement and waterproofing integrity should be combined; for industrial metals, corrosive environments, edges and defects should be combined; for outdoor floors, wear, impact and interlayer stability should be combined.
This article is a technical analysis and R&D evaluation suggestion supported by public information. It does not mean that Gaodun has completed all the tests listed. Specific model performance, compatible system and applicable substrate are subject to the corresponding technical instructions and test reports.
Further reading and technical information
The links below provide background on the topic. When it comes to specific performance, product selection or engineering parameters, please check the applicable objects and test conditions of each data.
- ASTM D7234-22: Pull-off strength of coatings on concrete and failure modes (store.astm.org)
- ISO 4624:2023: pull-off test for adhesion of coatings (iso.org)
- Journal of Elastomers & Plastics (2025): Preparation and properties of silicone modified polyurea materials (doi.org)
- Construction and Building Materials (2025): Interface shear between modified polyaspartic polyurea and concrete (doi.org)
The above original data is used to verify the corresponding technical principles, research formulas or construction examples, and is not the testing or certification of Gaodun products. Research conclusions should be understood together with formulas, specimens and test conditions; construction parameters of products from different manufacturers cannot be directly interchanged.