POLYASPARTIC TECHNICAL ARTICLES
Polyaspartic Polyurea Technical ArticlesHigh-Solids and Low-VOC Design in Polyaspartic Polyurea: From Formulation Metrics to Effective Film Formation
To assess an applied high-solids or low-VOC coating, measure dry film thickness and check the cured film for continuity. Solids data help estimate consumption. A VOC result applies to the material as tested. Neither figure establishes that the installed coating meets its thickness requirement or is free of pinholes and missed areas.
Article contents (9 sections)
1. What questions do high solids, solvent-free and low VOC answer respectively?
Polyaspartic polyurea usually relies on the reaction of polyaspartic ester resin containing secondary amine groups with isocyanate components for film formation. This reaction-curing path provides design space for reducing the amount of traditional volatile solvents. The Pasquick technical information disclosed by Covestro also links the polyaspartic ester system with reducing VOC emissions and improving construction efficiency. Covestro
However, the potential of technical routes does not mean that all formulations have the same environmental performance.
| concept | Main questions answered | Matters that cannot be proven independently |
|---|---|---|
| high solids | How much substance remains in the non-volatile fraction when measured according to the prescribed method? | Not established by this evidence alone: The same wet film can produce the same dry film |
| solvent-free | Does the formulation use conventional volatile solvents, and what is the scope of the claim? | Not established by this evidence alone: The measured VOC must be zero |
| Low VOC | Does the measured VOC content, using the specified method, meet the limit for the relevant product category or procurement requirement? | Not established by this evidence alone: Release performance after curing must meet indoor requirements |
| low release | How much does the material release into the air under specified conditions? | Not established by this evidence alone: Products have a low carbon footprint |
Gaodun advocates that product technical information should allow these terms to correspond to clear test objects, conditions and results respectively, so that customers can compare specific products.
2. Why are solids by mass and solids by volume not interchangeable?
Solids by mass express the mass fraction of nonvolatile material. Solids by volume express the fraction of the coating volume that forms dry film. The densities of pigments, fillers, resins and volatile components are different, making the two not directly equivalent.
ISO 3251:2019 provides a method for determining the mass content of non-volatile substances, and points out that the results are affected by factors such as heating temperature and time. Therefore, embedded data need to describe both the methods and conditions used. Determination of non-volatile-matter content
For engineering usage, the relationship between volumetric content and film thickness is more direct. Using matching volumetric solid content data, a theoretical estimate can be made under the conditions of flat substrate surface, uniform coating and neglecting construction losses:
Theoretical dry film thickness ≈ wet film thickness × volume solid content fraction.
For example, if the wet film thickness is 500 microns and the volume solid content is 90%, the theoretical dry film thickness is approximately 450 microns. This is a calculation example and does not represent the test results of a certain Gaodun product.
If all that is known is "90% solid content", the above dry film thickness cannot be directly derived. When calculating the construction dosage in kilograms, data such as the density of the mixture are also required.
The comparison that is of practical significance to customers is how much material is needed to achieve the same qualified dry film thickness, rather than just comparing the price per kilogram of product.
This is also the first connection that needs to be established when high solids products move from laboratory indicators to engineering evaluation.
3. Solvent-free formula, why do we still need to detect VOC?
To verify a coating’s volatile organic compound (VOC) content, consult the test report for that model. Identify whether the specimen was an as-supplied component, the mixed coating or the diluted application mixture. Record the method, result and unit. A solvent-free formulation description alone provides no measured VOC result.
Therefore, "no conventional solvents were actively added" and "the VOC measured according to the specified method is lower than a certain value" belong to two types of evidence.
ISO 11890-2:2020 and its 2024 amendment deal with the determination of VOCs and SVOCs in coatings using gas chromatography. When reading the report, you should check the standard version used, the reporting unit and the sample status. In particular, you should confirm whether the two components have been mixed according to regulations and whether they contain the diluent allowed to be added on site.ISO 11890-2:2020 Official Introduction (iso.org)and2024 Amendment (iso.org)。
For reactive two-component coatings, the data should also indicate whether Part A, Part B, or materials mixed according to the specified proportion are being tested; the time from mixing to sampling should also be controlled.
Gaodun believes that a complete low VOC statement should at least include product model, mixing ratio, detection method, result unit and whether on-site dilution is allowed. Such information is easier to verify than a single "environmentally friendly" label.
Particular attention needs to be paid to the construction state: if additional thinners are added on site, the data in the original packaging state are not sufficient to fully describe the actual construction material.
4. Reactive diluents reduce viscosity and also participate in determining the coating film structure.
Traditional non-reactive solvents mainly leave the coating through volatilization; active diluent components are designed to participate in the curing reaction and become part of the film formation structure.
However, "capable of reaction" does not mean that it can be completely transformed under any mixing ratio and construction conditions.
In the polyaspartic polyurea system, when a reactive low-viscosity component is introduced, its active hydrogen equivalent, functionality, reaction speed and compatibility need to be simultaneously investigated. It may change the original A/B ratio, or it may change the network connection method.
After changing a reactive diluent, prepare specimens of the revised formulation and record the mixing ratio, film thickness and cure conditions. To compare shrinkage or flexibility, test the original and revised formulations under matching conditions. Raw material functionality alone cannot establish a result for the finished coating.
Therefore, low viscosity is not the only evaluation criterion for active diluent components. Also to be answered: Is it effective in engaging reactions? Does it change the water resistance, media resistance and mechanical properties? Does it affect storage stability?
The research and development goals of active dilution should include application viscosity, effective conversion and final performance, and the three need to be verified together.
5. The key to high solids formula is to coordinate flow and solidification.
When assessing a reduced-solvent formulation, record the mixing ratio, material temperature, elapsed time after mixing and application method. On a representative substrate, examine wetting, levelling and residual bubbles before judging suitability for the proposed application.
To compare working time, record how long each mixture remains usable at the same temperature and mixed quantity. Check sagging on a vertical test panel and consult the model-specific technical data sheet (TDS) for the recoat interval. Record working time, vertical sag and recoat interval separately.
Increasing the application temperature can reduce the initial viscosity and may also speed up the reaction. Therefore, a single point viscosity at a certain temperature cannot fully describe the workability.
Gaodun's R&D judgment is that attention should be paid to the "construction window that changes over time": under the target temperature, mixing amount and construction method, whether the material can continue to complete wetting, leveling, and foam removal, and form a continuous coating within the required thickness range.
This requires the prepolymerized structure of Part A, the reactivity of Part B, and the collaborative design of the pigment, filler, and additive systems.
The difficulty of high solids technology is to make materials that rely less on volatile solvents still have stable and repeatable construction performance.
6. High solids does not mean that the thickness of a single pass can be increased infinitely.
At a given wet-film thickness, a higher volume solids fraction gives a greater theoretical dry-film thickness. Mass solids alone cannot determine that thickness. Other factors still limit the permitted thickness per coat.
If a thick test coat develops bubbles, record the substrate and its moisture condition, material temperature, time since mixing, wet film thickness of the coat and bubble locations. Compare test panels made from the same batch. A photograph of bubbles alone cannot identify the gas source.
It can be seen that even if the formula reduces solvent evaporation, the actual thick coating ability still needs to be evaluated.
For roofing, flooring and industrial protective coatings, the recommended single-coat thickness, recoating time and corresponding film formation quality should be verified separately. Local accumulation thickness should also be included in construction control.
Field acceptance requires both a dry film thickness measurement record and a cured film continuity inspection record. Identify the substrate, measurement locations and thickness in the first. Record any pinholes or missed areas in the same application area in the second. High solids or low VOC alone establishes neither result.
7. Low VOC content, low odor and low release should be evaluated separately
VOC content describes the content of relevant components in the material; release evaluation describes the material's behavior of releasing substances to the environment under specified conditions. The two are related, but the detection objects and time dimensions are different.
Smell is also not a substitute for the above tests. There are differences in the olfactory thresholds of different substances, and the intensity of odor cannot be directly converted into VOC content.
Therefore, for applications such as indoor floors, product evaluation needs to be combined with clear release test conditions, including sample preparation, curing time, test environment and sampling time points.
Low VOC cannot directly introduce low carbon. Evaluating carbon footprint also needs to consider boundaries such as raw materials production, transportation, construction energy consumption, maintenance and service life.
For Gaodun, explaining different environmental indicators separately helps customers select materials based on project goals, and also makes product technical expressions more verifiable.
8. How does Gaodun transform its formula advantages into engineering value?
Gaodun believes that the research and development value of high solids and low VOC technology should be implemented in verifiable product data and construction results.
| evaluation level | Important information | Significance to engineering |
|---|---|---|
| Recipes and raw materials | Reaction equivalent, raw materials composition, dilution component properties | Supports proportioning and curing structure design |
| Mixed construction status | Mixing ratio, temperature, viscosity change, allowable dilution | Clarify construction conditions |
| effective film formation | Volumetric inclusion, dry film thickness, continuity and defects | Evaluate actual coverage and protection effects |
| environmental performance | VOC content, release testing and conditions when necessary | Support application-specific environmental assessments |
| Usage performance | Applicable indicators such as adhesion, wear resistance, weather resistance or media resistance | Confirm performance balance after recipe adjustments |
For subsequent research and development, Gaodun is focusing on synergizing molecular structure and formula to reduce dependence on volatile solvents while maintaining an applicable construction window and long-term performance.
For polyaspartic polyurea, technological progress should be reflected in a more accurate expression of performance: Under clear construction conditions, a qualified coating is formed with a verifiable amount of material, and its environmental performance is explained with corresponding evidence.
Further reading and technical information
The links below provide background on the topic. When it comes to specific performance, product selection or engineering parameters, please check the applicable objects and test conditions of each data.
- ISO 3251:2019: Non-volatile substances content and method limits (committee.iso.org)
- Covestro: Pasquick polyaspartic ester technical data (solutions.covestro.com)
The above original data is used to verify the corresponding technical principles, research formulas or construction examples, and is not the testing or certification of Gaodun products. Research conclusions should be understood together with formulas, specimens and test conditions; construction parameters of products from different manufacturers cannot be directly interchanged.